Material

Uncoated

Coated

P-Value

Fuji II LC

Vertical loss

0.53 \(\pm\) 0.47

0.69 \(\pm\) 1.74

Volume loss

1.48 \(\pm\) 0.48A

2.12 \(\pm\) 1.75A

0.966

Ketac nano

Vertical loss

0.50 \(\pm\) 0.12

0.55 \(\pm\) 0.17

Volume loss

0.65 \(\pm\) 0.12B

0.76 \(\pm\) 0.17B

0.368

Equia forte fil

Vertical loss

0.37 \(\pm\) 0.21

0.65 \(\pm\) 5.49

Volume loss

0.95 \(\pm\) 0.21A

1.70 \(\pm\) 5.49A

0.333

Riva self cure

Vertical loss

0.76 \(\pm\) 2.15

0.60 \(\pm\) 1.79

-

Volume loss

1.52 \(\pm\) 2.15A

1.47 \(\pm\) 1.79AB