Table 2 Microhardness (HV) for tested group at 1 day and at 1 month post-photocuring

From: Effect of contamination of bulk-fill flowable resin composite with different contaminants during packing on its surface microhardness and compressive strength: in vitro study

 

One-day

One-month

p-value

n

Mean ± SD

95%CI

n

Mean ± SD

95%CI

Control

15

76.73a ± 4.57

74.85–78.62

15

76.16a ± 2.35

74.87–77.45

0.601

A. Saliva

15

75.00ab ± 2.45

73.11–76.88

15

75.78a ± 2.13

74.49–77.07

0.478

Alcohol

15

72.23b ± 5.26

70.34–74.11

15

75.81a ± 2.61

74.52–77.10

0.002

Gloves powder

15

74.58ab ± 2.62

72.69–76.46

15

75.44a ± 2.61

74.15–76.73

0.432

Hemostatic agent

15

73.90ab ± 2.39

72.01–75.79

15

74.92a ± 2.78

73.63–76.21

0.355

p-value

 

0.024

 

0.718

 