Skip to main content

Table 3 For each restorative material, the mean (± SD) µSBS obtained at the end of each setting time between the FSCSC and the restorative material

From: Delayed vs. immediate placement of restorative materials over Biodentine and RetroMTA: a micro-shear bond strength study

Restorative Material

FSCSS

Time

3 min (MPa ± SD)

12 min (MPa ± SD)

24 h (MPa ± SD)

Resin Composite

RetroMTA

1.48 ± 0.16 A

2.38 ± 0.163 A

3.61 ± 0.398 A

Biodentine

1.84 ± 0.241A

6.03 ± 0.644 B

6.37 ± 0.428 B

Theracal LC

RetroMTA

1.17 ± 0.095 A

1.28 ± 0.136 A

1.51 ± 0.138 A

Biodentine

1.11 ± 0.0852 A

1.38 ± 0.0954 A

1.64 ± 0.21 A

EQUIA Forte HT

RetroMTA

0.882 ± 0.072 A

1.05 ± 0.097 A

1.51 ± 0.19 A

Biodentine

0.924 ± 0.123 A

1.26 ± 0.154 A

1.67 ± 0.154 A

  1. Means sharing a superscript letter are not significantly different (p > 0.05)
  2. Per restorative material, letters compare column wise the mean µSBS obtained between the FSCSCs and each restorative material separately per setting time